Zinc-aluminium-magnesium (Zn-Al-Mg) coated steel is sheet steel that has been passed through a molten bath of zinc alloyed with small amounts of aluminium and magnesium, leaving a metallic coating that protects the steel both as a barrier and sacrificially. The coatings are sold under trade names such as ZAM and Magnelis and are designated ZM in European and Australasian standards.123 They are a sub-topic of steel roofing, sitting alongside the two long-established metallic coatings for roofing steel: zinc (galvanised, Z) and 55 percent aluminium-zinc (AZ, sold as Galvalume and Zincalume).
Zn-Al-Mg coatings are used for roof and wall sheeting (usually pre-painted), purlins and framing, rainwater goods and accessories, agricultural buildings, solar mounting structures and infrastructure.123 Their selling points are corrosion resistance at a lower coating mass than galvanising, a degree of self-protection at cut edges and scratches, and good performance in alkaline and ammonia-rich environments where aluminium-zinc coatings are weaker.
Chemistry and designations
The family covers a range of compositions. Australian standard AS 1397:2011 defines its ZM coating class as a continuously hot-dipped zinc coating with 5 to 13 percent aluminium, 2 to 4 percent magnesium and under 1 percent of minor control elements.13 Typical commercial products include:
- about 6 percent aluminium, 3 percent magnesium, balance zinc (the ZAM product developed by Nisshin Steel of Japan, now supplied in Australasia);3
- about 3.5 percent aluminium, 3 percent magnesium, balance zinc (93.5 percent), a European product;2
- higher-alloy versions with about 10 to 13 percent aluminium and 4 to 6 percent magnesium, and lower-alloy versions with about 1 to 3 percent aluminium and 2 to 4 percent magnesium.4
In Europe, the continuous hot-dip coating standard EN 10346 was extended in July 2015 to include zinc-magnesium coatings, which are designated ZM followed by the total coating mass on both faces in g/m².2 In Australia and New Zealand, ZM coating classes are specified under AS 1397 (and AS/NZS 1397); in New Zealand, ZM 240 is used as a substrate for coil-coated (pre-painted) products and ZM 450 for unpainted products.1
Under the microscope the coatings consist of zinc grains with eutectic mixtures of zinc, aluminium and zinc-magnesium intermetallic phases such as MgZn₂ and Mg₂Zn₁₁.4
How it protects the steel
All zinc-based coatings protect steel in two ways: as a physical barrier, and by corroding sacrificially where the steel is exposed. The aluminium and magnesium change the corrosion products that form. On zinc-aluminium coatings without magnesium, the main products are zinc oxide and zinc hydroxychloride (simonkolleite). With magnesium present, laboratory studies find layered double hydroxides of magnesium, zinc and aluminium, together with magnesium hydroxide; the magnesium acts as a pH buffer and pushes the chemistry away from loose zinc oxide toward these denser, more protective products.4 In a cyclic salt-spray test, for example, panels with about 2 to 4 percent magnesium showed around 8 percent rusted area and panels with 10 to 13 percent aluminium and 4 to 6 percent magnesium around 3 percent, compared with about 50 percent for a zinc-aluminium reference after the same exposure.4
In practice the coating develops a thin, tightly bonded aluminium-magnesium-rich surface film over time, giving a two-layer structure that slows corrosion of the coating itself.3
Cut-edge behaviour
Roof sheets are sheared, slit and drilled after coating, which leaves bare steel at every cut edge and hole. Cut edges are vulnerable because they expose steel, have thinner coating near the edge, and may crack during cutting.4 On Zn-Al-Mg coated sheet, cut edges first show red rust, which gradually darkens to grey-black as zinc-rich corrosion products spread over the exposed steel; after that the steel is protected sacrificially.3 This is the basis of the "self-healing" description used in marketing. The rate depends on exposure: in a salt-spray comparison one producer reports better red-rust resistance at cut edges than heavier hot-dip galvanising and performance comparable to 55 percent aluminium-zinc at bent edges.3
Comparison with galvanised and aluminium-zinc
| Galvanised (Z) | Aluminium-zinc (AZ) | Zinc-aluminium-magnesium (ZM) | |
|---|---|---|---|
| Coating | Zinc with trace aluminium | About 55% aluminium, balance mainly zinc | Zinc with about 1-13% Al and 1-6% Mg |
| Main protection | Sacrificial | Barrier (aluminium) plus some sacrificial | Barrier film plus sacrificial |
| Cut edges | Good sacrificial protection | Weaker, edge creep possible | Good |
| Ammonia, alkaline contact | Moderate | Weak | Good |
Producers claim that a ZM coating gives at least three times the corrosion resistance of galvanising at the same coating mass, or matches galvanising with a much thinner coating; one European producer claims up to ten times the atmospheric corrosion resistance of ordinary galvanised steel.23 In one sulfur dioxide test a 190 g/m² ZM coating outperformed a 550 g/m² galvanised coating by about six times, and the harder coating also resisted scratching better.3 In 24-hour exposure to 5 percent ammonia solution and to concrete extract at pH 11.5, ZM coatings lost less coating than galvanised steel; in acid and alkaline solutions generally, they behave much like other zinc coatings.3 Lower zinc loss also means less zinc in runoff to soil.2 Such figures come from accelerated laboratory tests and producer data, and real service life depends on the exposure.
Roofing uses
ZM-coated steel enters roofing in three main ways:
- Pre-painted sheeting. In New Zealand the coating is more commonly supplied as a factory pre-painted product than as bare sheet, roll-formed into corrugated, trapezoidal and standing-seam profiles.1
- Unpainted accessories and rainwater goods. Bare ZM has been used for roofing accessories and rainwater products.1
- Structure. Purlins, battens, top-hat sections and composite decking are widely made from ZM-coated steel, including in corrosive buildings.3
Recommended environments in producer literature include coastal and salt-prone sites, marinas and boat sheds, farm buildings, animal barns and composting sheds (where ammonia attacks aluminium-zinc), refineries and humid industrial buildings, and pool and spa enclosures.3
Limitations and good practice
- Galvanic corrosion. Like other zinc coatings, ZM is not protected from bimetallic corrosion. It should not be used with copper or receive runoff from copper.3
- Approximate lifespans. Because performance varies widely with exposure, producers present service-life estimates as approximate and refer designers to their technical manuals and national codes.31
- Repairs and fabrication. The coating can be welded, touched up with zinc-rich paint and painted much like galvanised steel.3
- Appearance. Bare ZM is bright when new and weathers to a satin, matt grey.3
- Chlorides. Laboratory work suggests that prolonged chloride exposure may eventually break down the magnesium-rich products, so ZM is not immune in severe marine conditions.4
History
Zinc-aluminium-magnesium coatings were developed in Japan, where Nisshin Steel introduced its ZAM product, and spread to Europe and Australasia in the following decades.3 European standardisation followed in 2015 with the inclusion of ZM coatings in EN 10346.2 The coatings are now produced by many steelmakers worldwide and appear in national roofing codes of practice; New Zealand's metal roofing code of practice, for example, includes durability clauses that address ZM coatings.1
Sources
Reviewed 2 November 2026 · 4 sources · 4 cited inline · Editorial policy · Plain-text version · Suggest a correction
- ZM CoatingsMetal Roofing Manufacturers New Zealand · metalroofing.org.nz
- ArcelorMittal's Magnelis compliant with European normSpecification Online · specificationonline.co.uk
- ZAM brochureStramit Building Products · media.architectureau.com
- Corrosion products of Zn-Al-Mg coatings in cyclic corrosion testingCoatings (MDPI) · mdpi.com