# Fire-Retardant-Treated Wood Shingles and Shakes

> Cedar shingles and shakes pressure-impregnated with leach-resistant fire-retardant chemicals so that, alone or over a specified underlayer, they meet Class B, C or A roof-covering fire ratings.

- URL: https://roof.wiki/fire-retardant-treated-wood-shingles/
- Topic: Roofing Materials
- Also known as: FRT shakes; FRT shingles; fire-retardant cedar shakes; fire-treated wood shingles; Certi-Guard; fire rated cedar roofing
- Regions: North America
- First published: 2026-11-02 · Last reviewed: 2026-11-02
- Cite as: "Fire-Retardant-Treated Wood Shingles and Shakes." roof.wiki. https://roof.wiki/fire-retardant-treated-wood-shingles/

## Key facts

- **Treatment:** Pressure impregnation, then kiln drying to fix the retardant
- **Product ratings:** Class B or Class C (ASTM E108 / UL 790)
- **Class A route:** Class B wood over gypsum roof board or ASTM D3909 cap sheet
- **Weathering test:** ASTM D2898 Method A: 12 weekly wet-dry cycles (84 days)
- **US evaluation criteria:** ICC-ES AC107 classified wood roof systems
- **Minimum slopes:** Shakes 4:12; shingles 3:12
- **Fasteners:** Stainless steel Type 304 or 316 (per evaluation)
- **Field study:** Most treatments still passed Class C burning-brand after 10 years

Fire-retardant-treated (FRT) wood shingles and shakes are sawn cedar shingles or split and sawn shakes that have been impregnated under pressure with fire-retardant chemicals and then kiln-dried to fix the chemicals in the wood.[5] Untreated wood roofing is combustible and is generally unrated or limited to the lowest fire classes, which has led many jurisdictions, particularly in wildfire-prone regions, to restrict it. Treatment allows cedar roofs to achieve Class B or Class C ratings as products and Class A ratings as part of tested roof systems.[1][2][6]

The topic is a sub-topic of [wood roofing](/wiki/wood-roofing), [wood shingle](/wiki/wood-shingle) and [wood shake](/wiki/wood-shake). It is closely related to preservative treatment, which protects wood against decay rather than fire; the two treatments are separate products and cannot be combined in the same shingle.[2]

## How treatment works

Treatment plants force a fire-retardant solution into graded cedar in a pressure vessel. Pressure impregnation gives much deeper penetration and higher chemical retention than brushing or dipping.[5] The shingles are then dried in a kiln at elevated temperature, which fixes (polymerises) the retardant so that it resists leaching.[5] Commercial formulations are proprietary, and some products are made at more than one retention level: one evaluated range offers Class B and Class C versions, with higher chemical retention for Class B.[6]

Only good stock is treated. Premium and No. 1 grade shakes and shingles are used, with lower-grade material reserved for starter courses.[2][6] Treatment is applied at a maximum moisture content, for example 25 percent in one evaluation.[6]

## Why exterior treatments must resist leaching

On a roof, fire retardant is attacked in two ways: rain and moisture leach soluble chemicals out of the wood, and weathering erodes the wood fibres and the chemicals they hold.[5] Retardants used outdoors must therefore be special non-leaching formulations.[3]

To prove durability, treated wood is weathered before it is fire-tested. ASTM D2898 sets out accelerated weathering methods; Method A, the one normally specified for regulatory purposes for exterior use, runs for twelve weeks (84 days), each week consisting of 96 hours of fine water spray at about 0.7 in (18 mm) per hour, using water at 35 to 60 °F (2 to 16 °C), followed by 72 hours of drying at 135 to 140 °F (57 to 60 °C).[7] Other methods add ultraviolet exposure from sunlamps.[7] Only after this weathering is the material fire-tested; for exterior FRT wood in general, a flame-spread rating of 25 is required after weathering.[3]

Field studies have shown why the weathering step matters. A US Forest Products Laboratory study tested fire-retardant-treated shingles after 0, 2, 5 and 10 years of outdoor exposure: after 10 years most treatments still passed the Class C burning-brand test of ASTM E108, but they had lost considerable effectiveness in a flame-spread test, and a commercial control treatment performed best.[4]

## Fire classes and assemblies

Roof coverings in North America are classified A (severe exposure), B (moderate) and C (light) under ASTM E108 / UL 790. For treated cedar:

- **Class C and Class B** are achieved by the treated shakes or shingles themselves, at the appropriate chemical retention, laid in the normal way.[6] In one evaluation, Class B and C assemblies of shakes add 36 in (914 mm) wide ASTM D226 Type II felt under the doubled starter course at the eaves.[6]
- **Class A** is reached by systems, not by the shingles alone. In the same evaluation, Class B shakes or shingles become a Class A roof when laid over spaced or solid sheathing covered with either 1/4 in (6 mm) gypsum-based roof board fastened with at least four fasteners per board, or a mineral-surfaced cap sheet to ASTM D3909 lapped 2 in (51 mm) at sides and ends; fasteners are lengthened to pass through the extra layer.[6]

The Cedar Shake and Shingle Bureau's roof manual notes that its fire-retardant-treated products can be used in Class A, B and C roof systems.[1] In Canada, permanent fire-retardant cedar products provide Class B and C ratings.[8]

## Codes and approvals

In the United States, treated shakes and shingles are accepted under the International Building Code and International Residential Code wood-shake and wood-shingle sections through evaluation reports that apply ICC-ES acceptance criteria for classified wood roof systems (AC107).[6] Such reports set conditions of use:[6]

- the product may be used only where its fire class is permitted;
- a Class B product may be used on a roof requiring Class A only within the specified Class A assembly;
- minimum slopes are 4:12 for shakes and 3:12 for shingles;
- hip and ridge exposure may not exceed field exposure, and starter courses are doubled;
- fasteners are stainless steel (Type 304 or 316).

Bundles carry the grading agency's label plus a treater's label stating the product, fire class, inspection agency and evaluation report number; in one programme Class B labels are printed in red and Class C in blue, and starter-course bundles are marked for starter use only.[6] Production is inspected under a continuing third-party quality programme.[6]

Exterior FRT wood is also used for wall shakes and cladding on buildings where combustible cladding would otherwise be restricted.[3]

## Installation

Treated shakes and shingles are installed like untreated ones, following the bureau's roof manual and local code for sheathing, exposure and nailing, with these additions:

- **Fasteners.** Some fasteners are incompatible with treated wood; treaters specify stainless steel or hot-dip galvanised nails, and evaluation reports may require stainless steel.[2][6]
- **Underlayers.** Any gypsum board or cap sheet needed for Class A must be installed as tested, and the underlayment goes over it.[6]

## Maintenance and service life

Fire-retardant-treated roofs must be maintained and inspected over time.[5] South- and west-facing slopes weather faster than north- and east-facing ones.[5] Periodic surface finishes slow weathering; film-forming finishes such as 100 percent acrylic latex stains or paints perform best on FRT wood, while penetrating stains perform poorly because the polymerised retardant fills the wood's pores.[5] As with any cedar roof, debris, moss and ponding moisture shorten life, and old roofs with moss growth should be cleaned and treated.[2]

## Preservative-treated alternatives

Preservative pressure treatment with copper-based chemicals such as chromated copper arsenate (CCA) is used to extend cedar's resistance to rot and fungal decay, particularly in hot, humid climates and on low slopes; the Cedar Shake and Shingle Bureau's preservative-treated line carries a 30-year warranty in Canada.[2][8][1] Because fire-retardant and preservative treatments cannot be combined in the same product, owners in humid wildfire areas must choose between them or rely on Class A system construction beneath the wood.[2]

## Sources

1. New Roof Construction Manual (2020) — Cedar Shake and Shingle Bureau. https://www.cedarbureau.org/wp-content/uploads/2020/04/roof-manual-2020.pdf
2. Cedar roofing (Interface, August 2000) — IIBEC. https://iibec.org/wp-content/uploads/2000-08-obando-1.pdf
3. Exterior use of fire-retardant-treated wood — Canadian Wood Council. https://old.cwc.ca/wp-content/uploads/2019/03/Exterior-use-of-FRTW.pdf
4. Effectiveness of fire-retardant treatments for shingles after 10 years of outdoor weathering (FPL 474) — USDA Forest Service, Forest Products Laboratory. https://research.fs.usda.gov/treesearch/5830
5. Exterior Rated Fire Retardant Treated Wood — Surviving Wildfire (Cooperative Extension). https://surviving-wildfire.extension.org/exterior-rated-fire-retardant-treated-wood
6. ESR-1410 FSR FTX fire-retardant-treated shakes and shingles — ICC Evaluation Service. https://icc-es.org/wp-content/uploads/report-directory/ESR-1410.pdf
7. ASTM D2898-10 Standard Practice for Accelerated Weathering of Fire-Retardant-Treated Wood for Fire Testing (sample) — ASTM International (via iTeh). https://cdn.standards.iteh.ai/samples/73176/33a75b1c458f431e86f6a6b3144717a6/ASTM-D2898-10.pdf
8. Shingled Roofing Systems: Cedar Shakes & Shingles — Roofing Contractors Association of British Columbia. https://rpm.rcabc.org/index.php/Shingled_Roofing_Systems:_Cedar_Shakes_&_Shingles