# Copper Flashing

> Sheet copper formed into step, base, counter, apron, valley, chimney and through-wall flashings, valued on slate, tile and masonry work for its long life and solderability.

- URL: https://roof.wiki/copper-flashing/
- Topic: Roof Components
- Also known as: copper step flashing; copper counterflashing; copper chimney flashing; copper valley; copper cap flashing
- Regions: North America, Europe, Global
- First published: 2026-11-02 · Last reviewed: 2026-11-02
- Cite as: "Copper Flashing." roof.wiki. https://roof.wiki/copper-flashing/

## Key facts

- **Standard (US):** ASTM B370 copper sheet, H00 or O60 temper
- **Default weight:** 16 oz/ft² (0.55 mm, 0.0216 in)
- **Base flashing under slate or tile:** 20 oz/ft² recommended
- **Minimum wall upstand:** 4 in (step pieces); 8 in (continuous base flashing)
- **Solder:** ASTM B32, 50-50 tin-lead or lead-free equivalent
- **Compatible in contact:** Lead, stainless steel
- **Keep away from:** Aluminium, zinc, galvanised and Al-Zn coated steel (contact and runoff)

Copper flashing is sheet copper bent, cut and often soldered to seal the joints between a roof covering and walls, chimneys, valleys, penetrations and edges. It is one of the traditional premium flashing metals, alongside lead, and is used especially with long-lived roof coverings such as natural slate, clay tile and wood shakes, where the flashing should last as long as the roof itself.[6] This article covers copper flashings specifically; the general principles are in [roof flashing](/wiki/roof-flashing), and copper as a roof covering in [copper roofing](/wiki/copper-roofing).

## How copper differs from other flashing metals

Compared with galvanised steel and aluminium, copper is heavier and costs more, but can be soldered into one-piece watertight assemblies, is very ductile for dressing around complex shapes, and does not need painting. Compared with [lead](/wiki/lead-roofing), it is much lighter and stiffer for the same coverage, holds a crisp fold, and can be used in long lengths, but it is less malleable, so it has to be formed into shapes rather than dressed over undulating tiles.

The main constraint is compatibility. Copper is one of the more noble building metals, so it accelerates the corrosion of less noble metals that it touches or that its runoff reaches (see [galvanic corrosion](/wiki/galvanic-corrosion)).[4][5]

## Material and weights

In North America, architectural copper sheet is made to [ASTM B370](/wiki/astm-b370) and described by weight in ounces per square foot. The Copper Development Association's model specification calls for cold-rolled H00 temper, or soft O60 temper where needed for forming, with a default weight of 16 oz/ft², which is 0.0216 in (0.55 mm) thick.[3] Its detail recommendations include:

- **Cap, apron and counterflashing:** at least 16 oz.[1][2]
- **Base flashing:** 16 oz for shingle roofs; 20 oz (about 0.69 mm, 0.027 in) recommended for slate and tile.[1]
- **Crickets (chimney saddles):** at least 16 oz.[1]
- **Locking strips:** the same weight as the flashing they engage.[2]
- **Laminated through-wall flashing:** thin copper (3, 5 or 7 oz/ft²) bonded to fabric or fibreglass, specified with the masonry.[3]

## Types of copper flashing

### Step and chimney flashing

Where a sloping roof meets a wall or chimney, copper is used either as individual steps or as a continuous runner:[1]

- **Individual step flashings.** Each base piece is woven in with a course of roofing. It reaches 2 in (51 mm) above the top of its course, with its lower edge ½ in (13 mm) above the butts of the next course. Base flashing runs at least 4 in (102 mm) up the wall and 4 in onto the roof. Cap (counter) flashings cover at least 4 in of the base flashing, and no step in masonry should be more than three bricks high. See [step flashing](/wiki/step-flashing).
- **Single runner.** A continuous copper base flashing is installed before the roof covering, with a hooked edge on the roof side cleated at 12 in (305 mm) centres. It rises at least 8 in (203 mm) up the wall and is covered by a two-piece cap made of a receiver and a counterflashing.

On a chimney straddling the ridge, the lower side gets a copper apron covering the next course of shingles. A chimney wholly on one side of the ridge gets a copper cricket, either one piece or two pieces joined by a standing seam, to divert water around it. All joints between base flashing sheets and the apron are soldered.[1] See [chimney flashing](/wiki/chimney-flashing) and [chimney cricket](/wiki/chimney-cricket).

### Counterflashing and reglets

Counterflashing (cap flashing) is built into the wall and laps down over the base flashing, so the two can move independently. The CDA details several ways of fixing it:[2]

- a copper receiver built into a mortar joint, with the counterflashing locked into its exposed edge;
- a saw-cut or cast reglet into which the flashing is inserted, held with lead wedges and sealed, though this is awkward at inside corners;
- in existing brickwork, a mortar joint raked out at least 2 in (51 mm) deep to form the reglet;
- a receiver cast into concrete, with the cap flashing riveted or cleated at 12 in centres.

Counterflashing laps the base flashing by at least 3–4 in (76–102 mm), and base flashings rise at least 8 in up the wall and are cleated at no more than 12 in centres.[2] See [counter-flashing](/wiki/counter-flashing).

### Low-slope and flat-roof flashings

On low-slope roofs, copper base flashings are attached to the deck before the membrane is laid and rise at least 8 in up walls and curbs, with copper cap flashings over their top edges.[1] Where copper is used with bituminous membranes, the membrane's own flashing runs at least 10 in (254 mm) up the wall and is lapped at least 4 in by the copper.[2]

### Valley, apron, edge and through-wall flashings

Copper is also used for open and closed valleys, eaves and rake edges, gravel stops and copings. In the CDA specification, copings and gravel stops are cleated at 12 in centres on their inner edges, locked over continuous cleats on the outer edge, and seamed at no more than 10 ft (3 m) intervals.[3] Through-wall flashings in masonry, often laminated copper, are covered in the masonry section of a specification.[3]

## Joining, fastening and movement

- **Soldering.** Copper flashings are soldered with ASTM B32 solder, traditionally 50-50 tin-lead or a lead-free alloy of similar strength, using an approved flux. Acid flux residues are neutralised with a baking-soda solution and rinsed off.[3] See [soldering sheet-metal roofing](/wiki/soldering-sheet-metal-roofing).
- **Fasteners.** Fasteners are copper or another metal recommended as compatible; sealants must be tested for use on copper.[3]
- **Movement.** Long flashings and copings need expansion joints, preferably lapped or bayonet joints. Otherwise, intermeshing hooked flanges at least 1 in (25 mm) deep are filled with concealed sealant, and moving seams must not be fastened so tightly that they cannot slide.[3] See [thermal movement in metal roofs](/wiki/thermal-movement-in-metal-roofs).

## Compatibility with other metals

Copper performs well in contact with lead and stainless steel, but has a severe corrosive effect on steel, aluminium and zinc.[4] Direct contact with zinc, aluminium, aluminium-zinc coated steel (such as [Galvalume](/wiki/galvalume)) or galvanised steel should be avoided, and runoff alone can cause damage: dissolved copper carried onto aluminium or zinc surfaces sets up many tiny galvanic cells, so the metals do not have to touch.[4][5] This matters where copper flashings sit above aluminium gutters, galvanised or coated steel roofing, or zinc.

Where contact cannot be avoided, the CDA specification calls for separating the metals with a bituminous coating, a cold-applied asphalt mastic of about 15 mil (0.38 mm) dry film per coat, or another permanent separation.[3] Ordinary prepainted roofing steel is not coated heavily enough to act as such a barrier.[4] Condensate from rooftop equipment with copper coils can be a stronger electrolyte than rain and should be piped to drains rather than onto metal roofs.[4]

Lead-coated and tin-zinc-coated copper were developed partly to reduce staining from copper runoff, and were widely used for flashings and valleys on slate roofs and on shingle roofs where hidden flashings could not be painted.[6] See [coated copper](/wiki/copper-roofing).

## Runoff and staining

Water running off copper carries small amounts of copper salts, which can stain light-coloured stone, brick, mortar, wood and paint green. Designers route copper drainage away from vulnerable surfaces, or use coated copper where staining would be unacceptable (see [copper runoff staining](/wiki/copper-runoff-staining)).[4][6]

## Service life and failure modes

Typical problems with copper flashings are:

- splits at soldered joints and fatigue cracks in long flashings without expansion provision;[3]
- leaks at reglets where sealant has failed or lead wedges have loosened;[2]
- corrosion of adjoining aluminium or galvanised components;[4][5]
- thin or under-weight copper torn by ice or by slate fragments, which is why heavier copper is recommended under slate and tile.[1]

## Sources

1. 9.8 Stepped and Chimney Flashings — Copper Development Association. https://www.copper.org/applications/architecture/arch_dhb/arch-details/flashings_copings/chimney.php
2. 9.2 Counterflashing — Copper Development Association. https://www.copper.org/applications/architecture/arch_dhb/arch-details/flashings_copings/counterflashing.php
3. 14.5 Copper Flashing and Trim (guide specification) — Copper Development Association. https://copper.org/applications/architecture/arch_dhb/specifications/arch_specs/flashing_and_trim.php
4. Dissimilar Metal Corrosion technical bulletin — Metal Construction Association (via ATAS International). https://www.atas.com/wp-content/uploads/2019/07/071216-Dissimilar-Metal-FINAL2.pdf
5. Galvanic corrosion — BRANZ Build magazine. https://www.buildmagazine.org.nz/assets/PDF/B113-49-Galvanic-Corrosion.pdf